Extruded 15 vol.% SiCp/Al-Cu-Mg composite was friction-stir-welded (FSW) and subjected to subsequent post-weld T4-treatment. The formation of Cu2FeAl7 phase with Fe resulting from steel tool wear was identified at or near the SiC particle interfaces by using transmission electron microscopy, high-resolution electron microscopy and differential scanning calorimetry. Two types of Cu2FeAl7 phases were observed: a single crystal phase and a polycrystalline nanostructured phase. No elemental iron was detected. The formation mechanism of the Cu2FeAl7 phase is discussed. (C) 2007 Acta Materialia Inc. Published by Elsevier Ltd. All rights reserved.
部门归属
chinese acad sci, inst met res, shenyang 110016, peoples r china.;ma, zy (reprint author), chinese acad sci, inst met res, 72 wenhua rd, shenyang 110016, peoples r china;zyma@imr.ac.cn